About EN 10025:3 S460NL Steel Plate
-
The designation of the EN 10025:3 standard for S460NL shows that this is steel for structural purposes (S), with a minimum yield strength of 460 MPa (460) at 16mm thick and below. This classification has specified minimum impact energy values at temperatures not lower than -50 deg C (NL).
As well as S460NL we are stockists of plates to EN 10025:3 S460N.
Applications
- Bridges
- Grouted tees/grouted sleeves
- Pipe caps/pipe fittings
- Pipe lines
- Plate girders
- Pressure vessels
- Road tankers
Properties
Chemical Requirements
(cast analysis, % by mass, maximum permitted unless indicated otherwise)
c | Si | Mn | P | S | Al total | N | Cr | Cu | Mo | Nb | Ni | Ti | V | NB+Ti+V | Mo+Cr |
---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
0.20 | 0.60 | 1.00 – 1.70 | 0.025 | 0.020 | 0.020 min | 0.025 | 0.30 | 0.55 | 0.10 | 0.05 | 0.80 | 0.05 | 0.20 | 0.22 | 0.30 |
Tensile Requirements
Product thickness | Yield strength (MPA) min | Tensile strength (MPA) | Elongation min |
---|---|---|---|
up to 16mm | 460 | 540 – 720 | 17 |
16mm to 40mm | 440 | 540 – 720 | 17 |
over 40mm to 63mm | 430 | 540 – 720 | 17 |
over 63mm to 80mm | 410 | 540 – 720 | 17 |
over 80mm to 100mm | 400 | 540 – 720 | 17 |
over 100m to 150mm | 380 | 530 – 710 | 17 |
over 150mm to 200mm | 370 | 530 – 710 | 17 |
Impact energy values for the normalised condition
Longitudinal
-50°C | -40°C | -30°C | -20°C | -10°C | 0°C | +20°C |
---|---|---|---|---|---|---|
27 J min | 31 J min | 40 J min | 47 J min | 51 J min | 55 J min | 63 J min |
Impact energy values for the normalised condition
Transverse
-50°C | -40°C | -30°C | -20°C | -10°C | 0°C | +20°C |
---|---|---|---|---|---|---|
16 J min | 20 J min | 23 J min | 27 J min | 30 J min | 34 J min | 40 J min |